深圳品茶,上海水磨会所老店,福州喝茶vx联系方式

Company News Industry News

The Defects Caused By Improper Forging Process

2023-12-08
1. Large grains
Large grains are usually caused by excessively high initial forging temperature and insufficient deformation, or excessively high final forging temperature, or the degree of deformation falling into the critical deformation zone. The deformation of aluminum alloy is too large to form texture; the deformation temperature of superalloy is too low, and the formation of mixed deformation structure may also cause coarse grains. Coarse grains will reduce the plasticity and toughness of forgings, and the fatigue performance will be significantly reduced.

2. Uneven grains
Uneven grains means that the grains in some parts of the forging are particularly coarse, but some parts are smaller. The main reason for the uneven grain is that the uneven deformation of the billet makes the degree of grain breakage different, or the deformation degree of the local area falls into the critical deformation zone, or the local work hardening of the superalloy, or the local grain during quenching and heating Gross.

3. Chilling phenomenon
Due to low temperature or too fast deformation speed during deformation, and too fast cooling after forging, it is possible that the softening caused by recrystallization cannot keep up with the strengthening (hardening) caused by deformation, so that part of the forging remains cold deformation after hot forging. organization. The existence of this structure improves the strength and hardness of the forging, but reduces the plasticity and toughness. Severe cold and hard phenomena may cause forging cracks.

4. Crack
Cracks are usually caused by large tensile stress, shear stress or additional tensile stress during forging. The place where the crack occurs is usually the place where the billet has the largest stress and the thinnest thickness. If there are micro-cracks on the surface and inside of the blank, or there are structural defects in the blank, or the plasticity of the material is reduced due to improper hot working temperature, or the deformation speed is too fast, the degree of deformation is too large, and the plasticity index of the material is exceeded, then the roughing, Cracks may occur in processes such as drawing, punching, reaming, bending and extrusion.

5. Cracking
Cracks are shallow turtle-like cracks on the surface of forgings. In the forming of forgings, the surface subjected to tensile stress is most prone to such defects.

The internal factors that cause the cracks may be various:

①The raw materials contain too much fusible elements such as Cu and Sn.
② When heated at high temperature for a long time, there will be copper precipitation on the surface of the steel material, coarse surface grains, decarburization, or the surface after repeated heating.

③The sulfur content of the fuel is too high, and there is sulfur infiltrating the surface of the steel material.


ABOUT  KEVA
Keva Casting is a professional casting company that focuses on Construction, Machinery, Automobile, Hardware, Pipeline and many other industries.
We provide top quality products with the best service based on our complete production chain including our own mold design, advanced production techniques, and full management of the supply chain. Keva Casting has two factories located in Zhucheng, China's Shandong province.
We use "shell molding", which is a new technique that has been developed in recent years.This new technique has simplified production procedures and reduced air pollution compared with traditional sand casting and investment casting. Shell making and core making are faster to ensure production in enormous quantities. The dimensions and surface finishing are satisfactory for all kinds of industrial requirements. Besides supplying our own formwork & scaffolding systems, our casting products also supply OEM services in various industries.

主站蜘蛛池模板: 长治市| 广宗县| 农安县| 绥棱县| 康马县| 灵寿县| 芜湖县| 呼和浩特市| 临漳县| 夏津县| 大庆市| 曲阳县| 沅陵县| 吕梁市| 乐安县| 余干县| 满洲里市| 保山市| 旬邑县| 兖州市| 阜宁县| 石河子市| 新乡县| 田阳县| 桐乡市| 海城市| 吴江市| 苏州市| 临沭县| 扬中市| 永新县| 壤塘县| 余干县| 塘沽区| 平凉市| 西林县| 军事| 吉安县| 双桥区| 梨树县| 凤庆县|